Nondestructive Testing of Copper–Aluminum Busbars in EV Battery Packs Using Ultrasonic Phased Arrays

I present my research on a nondestructive evaluation technique for copper–aluminum busbars used in EV battery packs. The growing adoption of EVs has increased the demand for reliable power battery modules. Among the key components in an EV battery pack, the copper–aluminum busbar is a critical connector that transports current from the battery modules to the electric drive system. It is usually manufactured by ultrasonic welding of a copper sheet and an aluminum sheet. Welding defects in these busbars can lead to electrical losses, local heating, and even thermal runaway of the entire EV battery pack. Therefore, inspection of the welded interface is essential to ensure safety and performance. Traditional quality control methods rely on destructive tensile tests that can only be applied to sampled workpieces. Such sampling cannot guarantee that every busbar in an EV battery pack is sound. My work aims to develop an effective ultrasonic phased-array-based nondestructive testing method for this specific application.

In this article, I first introduce the ultrasonic testing theory and the phased-array principle. Then I describe an ultrasonic C-scan imaging method for weld-defect detection. I subsequently propose a spectral-analysis imaging method that improves robustness with respect to the copper-surface condition. Finally, I present the design of a complete water-immersion ultrasonic phased-array inspection system and verify the method on 240 actual EV battery pack busbar workpieces.

1. Fundamental Theory of Ultrasonic Testing

Ultrasound is a mechanical wave with frequency above 20 kHz. When it propagates through different media, its amplitude, velocity, and spectrum are affected by the acoustic properties of the media. For a harmonic wave propagating along the positive x-axis, the displacement at position x and time t can be expressed by the following wave equation:

$$ y = A \cos\left[\omega \left(t-\frac{x}{c}\right)\right] = A \cos(\omega t – kx) $$

where A is the displacement amplitude, ω is the angular frequency, c is the wave velocity, and k is the wavenumber given by k = 2π/λ. The acoustic pressure is related to the particle displacement through the medium density ρ. More important is the concept of acoustic impedance:

$$ Z = \rho c $$

When a longitudinal ultrasonic wave propagates perpendicularly from a medium with impedance Z1 into another medium with impedance Z2, the sound pressure reflection coefficient r and transmission coefficient t at the planar interface are:

$$ r = \frac{P_r}{P_0} = \frac{Z_2-Z_1}{Z_2+Z_1} $$

$$ t = \frac{P_t}{P_0} = \frac{2Z_2}{Z_2+Z_1} $$

The reflected amplitude strongly depends on the acoustic impedance mismatch. A tightly bonded metallic interface with no air gap or oxide layer will transmit most of the acoustic energy, whereas a defective interface containing voids or delamination will cause a stronger reflection. This relationship is the basis of my defect detection methodology.

Ultrasonic Phased Arrays

An ultrasonic phased-array probe consists of many small piezoelectric elements that can be individually excited with controlled time delays. By adjusting the time delays of the elements, the beam can be steered and focused at a chosen depth. The delay law can be derived from the geometric path difference between each element and the focal point. For I, a one-dimensional linear phased-array probe is suitable for inspecting the flat lap geometry of copper–aluminum busbars in EV battery packs.

Two common scanning modes are linear electronic scanning and sectorial scanning. In linear scanning, a fixed aperture of elements is moved along the array direction while each group electronically focuses at the same depth. In sectorial scanning, a fixed group of elements sweeps the beam across a range of angles without mechanical movement. Because the weld region of the busbar is shorter than the probe footprint and the surface is nearly flat, I select a linear-scanning configuration with a focused beam targeted at the copper–aluminum interface.

2. Acoustic Transmission Model for Copper–Aluminum Busbars

A typical copper–aluminum busbar in an EV battery pack has an aluminum sheet welded to a nickel-coated copper sheet. The total thickness is usually less than 3 mm, and the interface consists of a thin intermetallic layer. Figure 2-14 in the original thesis illustrates the ultrasonic transmission path, but I will summarize the model without relying on any figure number. An ultrasonic transducer, positioned in water at a fixed standoff distance, emits a longitudinal pulse toward the busbar. The first echo that returns to the transducer is the reflection from the water/copper interface. Part of the pulse transmits into the copper and reaches the copper/aluminum interface. The reflection from that interface returns through the copper and the water, becoming the second echo in the A-scan signal.

Let P0 be the incident sound pressure at the water/copper interface. The reflected pressure of the first echo is:

$$ P_{1r} = P_0 \, r_{w/cu} $$

and the transmitted pressure into the copper is:

$$ P_{1t} = P_0 \, t_{w/cu} $$

At the copper/aluminum interface, the transmitted pressure from the copper side undergoes reflection with an unknown coefficient rx. The pressure reflected back toward the copper/water interface is P2r = P1t rx. Then the pressure transmitted through the copper/water interface into the water after the second reflection is:

$$ P_{3t} = P_0 \, t_{w/cu} \, r_x \, t_{cu/w} $$

For an unwelded region, the interface between copper and aluminum is not metallurgically bonded; a thin water layer, air gap, or other weakly coupled medium may exist. The reflection coefficient at that region is denoted rcu/al. Therefore, the second echo pressure from an unwelded area is:

$$ P’_{3t} = P_0 \, t_{w/cu} \, r_{cu/al} \, t_{cu/w} $$

By taking the ratio of the two second-echo amplitudes, the unknown absolute values of the transmission and receiving coefficients cancel. This yields the relative ultrasonic reflectivity:

$$ \frac{P_{3t}}{P’_{3t}} = \frac{r_x}{r_{cu/al}} $$

In an ultrasonic C-scan image, the pixel grayscale value g is proportional to the received echo amplitude. Therefore, the relative reflectivity can be computed as:

$$ R_x = \frac{r_x}{r_{cu/al}} = \frac{g_w}{g_u} $$

where gw is the average gray level of a welded area pixel and gu is the average gray level of the corresponding unwelded background. This ratio is a normalized metric that indicates the quality of the weld. When the weld is good, the copper/aluminum interface is homogeneously bonded and transmission is high, so the reflected echo is low and the ratio is small. Conversely, when a welding defect exists, the interface acts as a stronger reflector and the ratio increases.

3. Ultrasonic C-scan Imaging for Weld Defect Detection

3.1 Division of Foreground and Background

In my C-scan method, the region scanned within the anvil footprint is referred to as the die area. This area contains both the welded region and the surrounding unwelded region. The weld head contains a matrix of weld teeth, e.g., 5 rows by 6 columns or other specifications. Each weld tooth produces a square-like embossed zone on the workpiece. For each tooth, the corresponding welded region is treated as a virtual pixel. The gray value of a virtual pixel is the mean gray level of all physical pixels inside the rectangle of that tooth:

$$ \bar{g}(u,v) = \frac{1}{S_c} \sum_{(i,j)\in S_c} g(i,j) $$

where Sc is the rectangular area in pixels and g(i,j) is the gray level at coordinates (i,j).

Because the weld head is larger than the closed pattern of teeth, a small gap is set between the tooth matrix and the outer edge to avoid the extruded aluminum flash. The unwelded region surrounding the welding area is partitioned into sub-rectangles. For a virtual pixel at the edge of the welding region, the corresponding background is obtained by weighted averaging of the three nearest background blocks. Based on the approximate Gaussian temperature distribution across the weld cross-section, I assign weights of 0.159, 0.682, and 0.159 to the outer, middle, and inner background blocks, respectively. For example, if the three neighboring background blocks are gb1, gb2, and gb3, the background value assigned to that virtual pixel is:

$$ g_{wb} = 0.159\,g_{b1} + 0.682\,g_{b2} + 0.159\,g_{b3} $$

For inner teeth, the background is recursively assigned from the outer layer inward. In this way, a complete background assignment matrix is constructed. The relative reflectivity for tooth number n is then:

$$ R_{w,n} = \frac{g_{w,n}}{g_{wb,n}} $$

Finally, the overall weld-interface reflectivity is the average of all N virtual-pixel reflectivities:

$$ R_w = \frac{1}{N} \sum_{i=1}^{r} \sum_{j=1}^{c} R_{w,ij} $$

This value provides an index that can be compared with an empirical threshold.

3.2 Adaptive Segmentation of the Welded Region

To determine which parts of the C-scan image actually correspond to metallurgical joining, I implemented an adaptive segmentation algorithm based on seeded region growing. The first step is automatic seed selection. I partition the die area into tooth-size rectangles. For each rectangular virtual pixel, I calculate the difference between its mean gray level and the corresponding background gray level. The pixel with the maximum difference is chosen as the center of the initial seed:

$$ S_0 = \arg\max_{(u,v)} \left[ \bar{g}(u,v) – g_{wb}(u,v) \right] $$

After choosing the seed, the algorithm needs a growth threshold. I use a local Otsu (maximum inter-class variance) threshold within a combined region that includes the seed rectangle and its immediate background. The Otsu threshold separates the merged region into foreground and background classes by maximizing the between-class variance:

$$ \sigma^2(t) = w_1(t) w_2(t) \left[\mu_1(t)-\mu_2(t)\right]^2 $$

where w1 and w2 are the fractions of pixels in the two classes and μ1 and μ2 are their mean gray levels. The resulting threshold gseedt is used as the region-growing stopping condition. Starting from the seed point S0, I iteratively compare the eight-neighbor pixels with gseedt. Any neighbor whose gray level is below the threshold is added to the growing region. The process continues until no more pixels can be added. This adaptive region growing algorithm provides accurate extraction of the actual welding area. Compared with conventional region growing or pure Otsu thresholding, it avoids over-segmentation and under-segmentation due to noise and uneven illumination.

3.3 Single Detection Parameters in C-scan Imaging

From the segmented welded region and the virtual-tooth reflectivity matrix, I compute three parameters that characterize the weld quality of a copper–aluminum busbar in an EV battery pack:

Parameter Symbol Definition
Effective weld-tooth count d Number of teeth whose reflectivity is below a specified threshold.
Welding area a Physical area of the segmented welded region, in mm².
Lamination/fit ratio j j = 1 − Rw, where Rw is the average relative reflectivity.

The welding area is obtained by counting the pixels in the region R and converting the pixel count to physical units:

$$ a = \frac{N_R}{P_n} $$

where Pn is the number of pixels per square millimeter. The fit ratio j represents the degree of interfacial contact. A well-bonded interface has low reflectivity and therefore a high fit ratio close to 1.

3.4 Experimental Validation and Limitations

I applied the C-scan imaging method to a set of 40 copper–aluminum busbar specimens. The weld teeth were arranged in a 6 by 9 matrix. After scanning, I loaded each specimen in a tensile test machine to obtain destructive validation. The measured parameters were plotted in a three-dimensional space using effective weld-tooth count, welding area, and fit ratio. Good products and defective products formed two distinguishable clusters, but two misclassifications occurred: one defective specimen was accepted and one good specimen was rejected.

Careful analysis revealed the cause of these misclassifications. The copper sheet is in contact with the anvil during ultrasonic welding, and the anvil leaves a network of small indentations on the copper surface. These indentations, whose depth and distribution vary from workpiece to workpiece, alter the amplitude of the first echo and the second echo independently. In the C-scan image, the unwelded background may appear darker or brighter than expected, causing the calculated reflectivity to be biased. Consequently, the fixed background reference from the unwelded region is not robust enough for all conditions found in an EV battery pack manufacturing environment. This motivated my second imaging method based on frequency-domain energy contrast.

4. Ultrasonic Spectral-Analysis Imaging

4.1 Energy Contrast Parameters

To suppress the influence of surface indentation, I define a spectral energy contrast parameter that compares the interface echo with the first water/copper echo in a self-calibrating manner. Both echoes undergo the same influence from the local copper-surface condition when they pass through the copper/water interfaces. Therefore, by taking the ratio of their energies in selected frequency bands, the surface condition is largely canceled.

Let x1(t) be the first echo from the water/copper interface and x2(t) be the interface echo from the copper/aluminum region. Their amplitude spectra are S1(f) and S2(f). I define three energy contrast parameters:

$$ R_{6dB} = \frac{\int_{f_{-6dB}}^{f_{+6dB}} S_2^2(f)\,df}{\int_{f_{-6dB}}^{f_{+6dB}} S_1^2(f)\,df} $$

$$ R_{h} = \frac{\int_{f_c}^{f_{max}} S_2^2(f)\,df}{\int_{f_c}^{f_{max}} S_1^2(f)\,df} $$

$$ R_{a} = \frac{\int_{f_{min}}^{f_{max}} S_2^2(f)\,df}{\int_{f_{min}}^{f_{max}} S_1^2(f)\,df} $$

Here, f−6dB and f+6dB define the 6 dB bandwidth around the center frequency, fc is the center frequency, and fmin and fmax are the lower and upper limits of the useful spectral band. In a defective weld, the interface echo is stronger because, at the defect location, there is a discontinuity: the incident wave cannot transmit into the aluminum sheet efficiently. The reflected wave has higher energy, and hence the value of the contrast parameter increases.

4.2 Improved VMD Denoising

The raw A-scan signals acquired from the ultrasonic phased-array system contain electronic noise and other disturbances. To denoise the signal, I use Variational Mode Decomposition (VMD) with parameters optimized by the Sparrow Search Algorithm (SSA). The VMD method decomposes a signal x(t) into a set of K band-limited intrinsic mode functions u_k(t), each with center frequency ω_k, by solving a constrained variational problem:

$$ \min_{\{u_k\},\{\omega_k\}} \sum_{k=1}^{K} \left\| \partial_t \left[ \left( \delta(t)+\frac{j}{\pi t}\right) * u_k(t)\right] e^{-j\omega_k t} \right\|_2^2 $$

$$ \text{subject to } \sum_{k=1}^{K} u_k(t) = x(t) $$

The augmented Lagrangian function is:

$$ \mathcal{L}(\{u_k\},\{\omega_k\},\lambda) = \alpha \sum_{k=1}^{K} \left\| \partial_t \left[ \left( \delta(t)+\frac{j}{\pi t}\right) * u_k(t)\right] e^{-j\omega_k t} \right\|_2^2 + \left\| x(t)-\sum_{k=1}^{K} u_k(t)\right\|_2^2 + \langle \lambda(t), x(t)-\sum_{k=1}^{K} u_k(t)\rangle $$

where α is the balancing parameter and λ is the Lagrange multiplier. The alternating-direction method of multipliers solves this problem iteratively.

The performance of VMD strongly depends on the modal number K. I use the minimum envelope entropy as the fitness function and SSA to optimize K. The improvement suppresses both noise and mode mixing, which is a common issue with empirical mode decomposition. I compared SSA-VMD with EMD, EEMD, and standard VMD on a noisy simulated signal. Mean values are summarized below.

Method SNR (dB) Root-mean-square error
EMD 11.94 1.27
EEMD 12.27 0.93
VMD 13.13 0.76
SSA-VMD 13.78 0.52

The optimized VMD achieves the highest signal-to-noise ratio and the lowest root-mean-square error, confirming its usefulness for subsequent frequency-domain feature extraction.

4.3 Multi-scale Echo Signal Segmentation

To compute the energy of different interface echoes, the A-scan signal must be split into the first echo and the subsequent interface echoes. In a water-immersion setup, the time-of-flight depends on the water path thickness, copper thickness, and their acoustic velocities. Owing to workpiece topology, the echo positions can vary slightly among scan points. A fixed time gate can be unreliable.

I developed a multi-scale segmentation method based on the Hilbert transform and a modification of Otsu’s thresholding. First, the Hilbert transform is applied to the denoised A-scan signal to obtain the envelope:

$$ \hat{x}(t) = \frac{1}{\pi} \int_{-\infty}^{\infty} \frac{x(\tau)}{t-\tau}\,d\tau $$

$$ A(t) = \sqrt{x^2(t)+\hat{x}^2(t)} $$

The envelope A(t) is then processed to locate the time position of its global maximum, which corresponds to the first echo from the water/copper interface. After this position, a search range is set from 1.5 to 2 times the round-trip time through the copper sheet. Within that range, I apply an OTSU-like threshold to determine the point that best separates the first echo from later echoes. Because the method adaptively selects both the horizontal position and the width of the echo window, it is robust to wavefront shifts caused by uneven busbar surfaces in EV battery pack production.

4.4 Imaging from Energy-Contrast Matrices

After denoising and segmentation for every scan position, I compute the chosen energy-contrast parameter. All values are arranged in a matrix according to the mechanical scan coordinates. The matrix is then rescaled to an 8-bit grayscale image by linear mapping so that the largest energy contrast becomes white and the smallest becomes black. The resulting spectral-analysis image is directly comparable to a conventional C-scan image, but the pixel values represent normalized frequency-domain energy ratios instead of raw time-gate amplitudes.

I tested three contrast metrics on a set of workpieces with different indentation states. The experimental results showed that the high-frequency contrast parameter Rh gave the best accuracy in both weld-area sizing and defect identification. Quantitative comparison for three representative workpieces is shown below.

Imaging parameter Workpiece 1 error (%) Workpiece 2 error (%) Workpiece 3 error (%)
R6dB imaging 8 9 11
Rh imaging 6 5 8
Ra imaging 7 6 10

The Rh parameter focuses on the higher-frequency portion of the ultra-sound spectrum, which is more sensitive to the fine interfacial condition of a thin copper–aluminum ultrasonic weld. Moreover, this band is less affected by the low-frequency reverberations from the large surface structure.

4.5 Detection Parameters Using Spectral-Analysis Images

When the spectral-analysis image is obtained, the same three parameters can be extracted. The effective weld-tooth count is determined by comparing the mean gray value inside each tooth rectangle with a threshold. The welding area is still obtained from the adaptive region-growing segmentation. The fit ratio is computed as one minus the normalized average reflectivity. Experimental validation on 40 additional specimens show an average error of less than 7% for both the effective weld-tooth count and the welded-area size, which confirms that the self-calibrated spectral contrast provides a reliable measure of the actual weld footprint.

5. System Design and Experimental Setup

5.1 Hardware Architecture

I designed and built a water-immersion ultrasonic phased-array inspection system for copper–aluminum busbars used in EV battery packs. The system consists of the following main modules:

Module Components Functions
Industrial PC Advanced IPC-610L, 32 GB RAM, Windows 10 Central control, signal processing, user interface
Motion control Inovance Easy500 PLC and servo motor Moves the probe, sends encoder pulses
Ultrasonic board MultiPulse ROBUST phased-array card Generates/receives pulses, collects A-scan data
Probe 15s64-0.5×10, 64-element linear array Emits and receives ultrasound waves
Water tank and fixture Custom stainless-steel tank and positioning jig Implements immersion coupling and consistent geometry

The ultrasonic board has a sampling rate of 100 MHz, an ADC resolution of 10 bits, and supports linear and sectorial scans. The 64-element linear probe has a center frequency of 15 MHz and element pitch of 0.5 mm. The PLC and servo motor provide precise positioning along the lateral scan axis.

5.2 Software Design

I developed custom software in C++ with Qt, running on the industrial PC. The software contains four main modules: parameter setting, data acquisition communication, imaging and signal processing, and result display. The parameter-setting module accepts workpiece dimensions, weld-tooth specifications, scan velocity, water delay, and focal depth. The result display module shows the weld map, highlights effective and ineffective weld teeth, and classifies the specimen as accepted or rejected.

5.3 Scanning Parameters and Inspection Procedure

The copper sheet thickness is 1.6 mm and the aluminum sheet thickness is 1.2 mm. The transducer is placed in water at a standoff distance of 20 mm. I choose a linear-scan mode with a 15 MHz focused beam at a focal depth of 5 mm. The key scan parameters are summarized below:

Parameter Value
Water path 20 mm
Wedge delay 11 μs
Focal depth 5 mm
Copper sound speed 4700 m/s
Aluminum sound speed 6300 m/s
Scan mode Linear electronic scanning
Aperture 4 elements
Start/end elements 1/64

During inspection, the servo motor moves the probe across the busbar. The ultrasonic board records one A-scan signal at every encoder pulse, together with the corresponding lateral coordinate. The software reconstructs the C-scan or spectral-analysis image after the scan is completed.

5.4 Defect Discrimination Model

I combine the three extracted parameters into a simple decision rule. Let Q be the final product status. If the effective weld-tooth count d, the welding area a, and the fit ratio j satisfy

$$ d \ge d_0, \quad a \ge a_0, \quad j \ge j_0 $$

the busbar is classified as a good product; otherwise it is classified as defective. The thresholds d0, a0, and j0 are determined empirically from the tens of samples destructively tested during the design phase.

6. Experimental Results

I carried out a comprehensive experiment using 240 copper–aluminum busbar specimens manufactured with different welding parameters such as energy, pressure, and amplitude. All specimens were first inspected by the ultrasonic phased-array system using both the C-scan imaging method and the spectral-analysis imaging method. Then I performed destructive pull tests to provide ground truth labels. The pull tests included both shear and peel configurations. Each specimen was classified as a good product or a defective product according to the tensile force and the residual weld area on the copper sheet. The ground truth data set included 200 good products and 40 defective products.

The table below provides representative data from selected samples, including the ultrasonic parameters and the destructive shear force.

Sample Effective teeth Area (mm²) Fit ratio Shear force (N) Status
1 48 98 0.95 1848 Good
2 49 102 0.96 1986 Good
3 50 100 0.95 2061 Good
4 51 103 0.96 2047 Good
5 46 99 0.89 1707 Good
6 44 92 0.86 1690 Good
7 2 62 0.69 967 Defective
8 3 64 0.72 976 Defective
9 4 71 0.75 1113 Defective
10 2 61 0.68 956 Defective

Because the acceptance of a defective busbar into an EV battery pack is the most dangerous type of error, I analyzed the results by defining two error types analogous to Type I and Type II errors in statistical hypothesis testing. Let α be the missed-defect rate (defective product accepted) and β be the false-rejection rate (good product rejected). They are computed as:

$$ \alpha = 1 – \frac{c_b}{N_b}, \qquad \beta = 1 – \frac{c_g}{N_g} $$

where cb is the number of defective products correctly detected, Nb is the total number of defective products, cg is the number of good products correctly detected, and Ng is the total number of good products.

The accuracy of the two ultrasonic methods is summarized below.

Method Correctly accepted goods Correctly rejected defects Good accuracy (%) Defect accuracy (%) α β
C-scan imaging 197 33 95.0 82.5 0.175 0.05
Spectral-analysis imaging 199 40 99.5 100.0 0.000 0.005

In the C-scan method, 7 out of 40 defective specimens were missed, resulting in a missed-defect rate of 17.5%. The spectral-analysis method did not miss any defective product. Meanwhile, only one good product out of 200 was rejected, yielding a false-rejection rate of 0.5%.

These results clearly demonstrate that the spectral-analysis imaging method is superior to conventional amplitude-gate C-scan imaging for detecting ultrasonic weld defects in copper–aluminum busbars. The improved method is self-calibrating because it compares the interface echo with the first surface echo, so variations caused by copper surface indentation are effectively canceled. This is especially important in mass production of EV battery packs, where the surface condition of busbars cannot be perfectly controlled.

For additional verification, I compared the effective weld-tooth count and the weld-area size obtained from the ultrasonic method with the physical measurements after destructive testing. The average error for the spectral-analysis method was less than 7% for both parameters. Some measured errors from the first 8 random samples are tabulated below.

Sample Effective tooth count error (%) Weld-area size error (%)
1 6 7
2 9 8
3 7 7
4 6 4
5 4 6
6 9 8
7 6 7
8 7 9

These deviations are acceptable for production-line quality assurance. The ultrasonic phased-array method is fast, automatic, and non-destructive, making it an attractive alternative to destructive pull testing for every busbar in an EV battery pack.

7. Conclusion and Outlook

In this study, I have addressed the challenge of non-destructive inspection of copper–aluminum busbars used in EV battery packs. I first described the fundamentals of ultrasonic testing and ultrasonic phased-array imaging. Then I proposed a complete processing chain that includes robust signal denoising, adaptive echo separation, and frequency-domain energy-contrast imaging. The main findings and contributions of my thesis can be summarized as follows.

First, I developed a C-scan reflectivity-calculation method based on the division of the weld area into virtual pixels corresponding to the weld teeth. I introduced a background-assignment matrix that models the influence of the weld heat distribution. I also designed an adaptive region-growing algorithm for weld-area segmentation using a local Otsu threshold. The C-scan method works in most cases, but the copper surface indentation left by the anvil can severely bias the reflectivity reference, leading to occasional misclassifications.

Second, I proposed a spectral-analysis imaging method that uses the energy ratio between the interface echo and the surface echo. This self-calibrating approach effectively removes the adverse influence of local surface indentation. I enhanced the signal quality by using SSA-VMD denoising. The improved method achieved a missed-defect rate of 0% and a false-rejection rate of only 0.5% on the 240 specimen validation set.

Third, I built a complete water-immersion ultrasonic phased-array inspection system and integrated it with custom software. The system is suitable for automatic online quality control of busbars in EV battery pack assembly lines.

Although my method has achieved promising results, there are still several directions for future improvement. Convolutional neural networks or other deep-learning models could be applied to the ultrasonic images to further improve weld-area segmentation and defect classification. The echo-segmentation step could also benefit from long short-term memory networks due to their ability to model time-series context accurately. In addition, the algorithm speed could be increased through parallel processing or FPGA-based hardware acceleration so that the system can inspect every busbar in an EV battery pack at full production speed.

In conclusion, ultrasonic phased-array spectral-analysis imaging provides a reliable and practical non-destructive evaluation tool for copper–aluminum busbar welds in EV battery packs. The self-calibrating energy contrast removes the surface condition influence and enables a fast, low-cost, and accurate inspection. I hope this work will contribute to improving the quality and safety of EV battery pack manufacturing.

Scroll to Top