As the demand for electric vehicles continues to grow, the safety and durability of the electric vehicle battery pack remain critical challenges. In my research, I focused on two primary abuse modes: electrical abuse and thermal abuse. I conducted a series of experiments on lithium iron phosphate (LFP) and ternary lithium-ion (NCM) cells under various ambient temperatures, ranging from −25 °C to 75 °C. I investigated overcharge behavior, high-rate overcharge, and thermal runaway during discharge. Through these experiments, I revealed the temperature-dependent performance differences, parameter variations, and failure mechanisms. The findings provide a foundation for improving the safety design of the electric vehicle battery pack.

I began by examining the overcharge failure mechanisms of LFP power batteries at different ambient temperatures. I used 23 Ah prismatic LFP cells with a nominal voltage of 3.2 V. Prior to testing, I performed three formation cycles at 0.5 C and selected cells with a capacity of 23 ± 1 Ah and an internal resistance of 5 ± 1 mΩ at 100% state of charge (SOC). I then subjected these cells to 1 C overcharge at −25, 0, 25, 50, and 75 °C until the vent valve opened. I monitored surface temperature and voltage using K-type thermocouples and a data logger at 1 Hz, and I recorded the entire process with a camera. Table 1 summarizes the key parameters of the LFP cells.
| Parameter | Value |
|---|---|
| Cathode | LiFePO4 |
| Anode | Graphite |
| Dimensions (mm) | 68 × 24.2 × 131 |
| Nominal capacity (Ah) | 23 |
| Nominal voltage (V) | 3.2 |
| Charge voltage (V) | 3.65 |
| Discharge end voltage (V) | 2.0 |
During overcharge, I observed four stages: initial polarization, gas accumulation and swelling, safety valve opening with white smoke, and cooling. As ambient temperature decreased from 75 °C to −25 °C, the venting duration increased and the amount of released gas increased. The voltage evolution exhibited strong temperature sensitivity. At low temperatures (−25 and 0 °C), five stages appeared; at room temperature (25 °C), four stages; and at high temperatures (50 and 75 °C), three stages. This indicates that higher temperatures accelerate the internal electrochemical reaction kinetics. The side reactions producing gas can be represented by the following equations:
$$ C_3H_4O_3 (EC) + 2Li \rightarrow Li_2CO_3 + C_2H_4 $$
$$ C_4H_6O_3 (PC) + 2Li \rightarrow Li_2CO_3 + C_4H_6 $$
$$ C_3H_6O_3 (DMC) + 2Li \rightarrow Li_2CO_3 + C_2H_6 $$
I also analyzed the boundary conditions and internal resistance changes. At 75 °C, the voltage surge occurred at only 295 s, and the maximum temperature difference reached 151.1 °C. This indicates that overcharge at extremely high temperatures leads to rapid failure and a high probability of thermal runaway. In contrast, at low temperatures, the risk of thermal runaway is reduced. Interestingly, the internal resistance first increased and then decreased during overcharge. When the positive temperature coefficient (PTC) protection mechanism was triggered, continued overcharge caused a decrease in internal resistance. Table 2 shows the internal resistance changes at different SOC levels for the LFP cells.
| Internal resistance change (mΩ) | −25 °C | 0 °C | 25 °C | 50 °C | 75 °C |
|---|---|---|---|---|---|
| 105% SOC | 0.892 | 0.041 | 0.587 | 1.085 | 1.324 |
| 110% SOC | 1.626 | 0.569 | 3.165 | 25.570 | 5.559 |
| 115% SOC | 2.590 | 2.924 | 247.360 | 32.639 | 80.728 |
| 120% SOC | 0.332 | 0.526 | 32.310 | 20.684 | 13.085 |
For the electric vehicle battery pack, these results imply that overcharge warning strategies should consider ambient temperature. The voltage surge point occurred at least 100 s before the maximum temperature point at all temperatures tested. Therefore, the voltage surge point can serve as an early warning indicator for overcharge-induced thermal runaway in LFP-based electric vehicle battery packs.
Next, I investigated the overcharge behavior of ternary lithium-ion batteries at different ambient temperatures. I used 26650 cylindrical NCM cells with a nominal capacity of 5 Ah and a nominal voltage of 3.6 V. Table 3 lists the cell parameters. After formation and capacity screening, I selected cells with a capacity of 4.95–5.05 Ah and an internal resistance of 21–23 mΩ at 100% SOC. I performed 3 C overcharge at −25, 0, 25, 50, and 75 °C until failure. I also conducted electrochemical impedance spectroscopy (EIS) and post-mortem microscopic characterization using scanning electron microscopy (SEM), energy-dispersive X-ray spectroscopy (EDS), and X-ray diffraction (XRD).
| Parameter | Value |
|---|---|
| Cathode | Li(NiCoMn)O2 |
| Anode | Graphite |
| Dimensions (mm) | 26 (D) × 65 (H) |
| Nominal capacity (Ah) | 5 |
| Nominal voltage (V) | 3.6 |
| Charge voltage (V) | 4.2 |
| Discharge end voltage (V) | 2.75 |
The voltage evolution during 3 C overcharge showed a clear dependence on ambient temperature. At −25 °C, six stages were identified; at 0 and 25 °C, five stages; and at 50 and 75 °C, only two stages. The lower the ambient temperature, the greater the maximum temperature difference during overcharge. This is because at low temperatures, the electrode surface resistance Rct and double-layer capacitance Cdl increase significantly, leading to more ohmic heat generation under constant current. The voltage surge point appeared fastest at 25 °C, and the time interval between the voltage surge point and the maximum temperature point was less than 40 s at all temperatures. This short interval poses a serious challenge for thermal runaway warning in an electric vehicle battery pack.
I also analyzed the internal resistance changes at different SOC levels. Table 4 presents the internal resistance changes for the NCM cells. At temperatures ≤ 25 °C, the internal resistance increased with SOC. At high temperatures (50 and 75 °C), the internal resistance decreased with SOC. The minimum corrosion of the current collector and electrolyte decomposition occurred at 25 °C. As the ambient temperature deviated from room temperature, the damage to the cathode and anode increased.
| Internal resistance change (mΩ) | −25 °C | 0 °C | 25 °C | 50 °C | 75 °C |
|---|---|---|---|---|---|
| 110% SOC | 0.007 | 0.001 | 0.001 | 0.003 | 0.003 |
| 120% SOC | 0.011 | 0.001 | 0.001 | 694.676 | 911.777 |
| 130% SOC | 443.08 | 363.576 | 352.076 | 481.478 | 573.276 |
| 140% SOC | 468.08 | 382.179 | 393.777 | 442.478 | 521.577 |
The EIS results showed that the ohmic resistance Rs increased with SOC at all temperatures, likely due to current collector corrosion and electrolyte decomposition. The charge transfer resistance Rct increased slightly with SOC, indicating minor electrode damage and separator pore blockage. At 110% SOC, the minimum Rs was observed at 25 °C, confirming that room temperature overcharge causes the least corrosion and decomposition. As the temperature deviated from 25 °C, Rs increased and then stabilized at extreme temperatures.
SEM images of the cathode revealed that at 110% SOC, the morphology changed little compared to 100% SOC. From 120% SOC onward, gaps appeared between particles, and these gaps became more pronounced at 130% and 140% SOC. This indicates that overcharge causes structural loosening of the cathode, likely due to oxidative decomposition of the PVDF binder. Irregular white bumps, attributed to cathode decomposition, increased with SOC and were more severe as the temperature deviated from 25 °C. EDS detected C, O, Ni, Co, and Mn in the cathode, showing that the active materials did not completely lose their elemental composition.
For the anode, SEM images showed that at 100% SOC, lithium metal particles adhered to the graphite surface. As overcharge progressed, the volume of lithium metal aggregates increased, and gaps appeared between particles. At 50 and 0 °C, the gaps were larger than at 25 °C, likely due to faster lithium aggregation at high temperature and weaker adhesion at low temperature. At 75 °C and −25 °C, the gaps were somewhat smaller than at 50 and 0 °C, respectively. EDS detected C and O in the anode, with C from graphite and O from lithium oxides and separator decomposition.
XRD analysis of the cathode showed that at 25 °C, the characteristic peak positions remained stable with increasing SOC, indicating good structural stability. At 50 and 75 °C, the (003) peak shifted to higher 2θ values, especially at 130% and 140% SOC, indicating deformation and collapse of the layered structure. For the anode, the LiC6 (001) peak remained stable at 25 °C, while the LiC12 (002) peak decreased with SOC up to 130% and then slightly increased at 140%, suggesting lithium plating after separator breakdown. At 50 °C, the LiC6 peak was highest, indicating maximum lithium insertion, but at 75 °C, severe electrode damage reduced the peak intensity.
These findings highlight that the safety of an electric vehicle battery pack depends strongly on ambient temperature. Overcharge at room temperature does not necessarily yield the best safety performance in terms of voltage surge timing, but it minimizes corrosion and decomposition. The electric vehicle battery pack management system should account for these temperature-dependent behaviors.
Finally, I studied the thermal runaway performance of ternary lithium-ion batteries during discharge at different ambient temperatures. I used the same 26650 NCM cells. I discharged them at 1 C and simultaneously heated them with a 120 W heating film until thermal runaway occurred. The ambient temperatures were −25, 0, 25, 50, and 75 °C. I recorded the entire process with a camera, took macroscopic photographs after thermal runaway, and performed SEM, EDS, and XRD on the ejected particles and the post-runaway electrodes.
The thermal runaway process could be divided into four stages based on voltage and temperature changes. Stage 1: heating and SEI decomposition. The SEI decomposition reaction is given by:
$$ (CH_2OCO_2Li)_2 \rightarrow Li_2CO_3 + C_2H_4 + CO_2 + 0.5O_2 $$
Stage 2: gas accumulation and safety valve opening. Stage 3: reaction between the anode and electrolyte, producing white smoke. The reactions include:
$$ 2Li + C_4H_{10}O_3 (DEC) \rightarrow Li_2CO_3 + C_2H_4 + C_2H_6 $$
$$ 2Li + C_3H_6O_3 (DMC) \rightarrow Li_2CO_3 + C_2H_6 $$
$$ 2Li + C_4H_6O_3 (PC) \rightarrow Li_2CO_3 + C_3H_6 $$
Stage 4: thermal runaway with intense flame ejection. The time from the voltage drop point (Vdp) to thermal runaway was at least 89 s at all temperatures. Therefore, Vdp can be used as a thermal runaway warning point in an electric vehicle battery pack. The safety valve opening point (TSVO) is not suitable because the interval to thermal runaway is too short, especially at high temperatures.
I observed that as the ambient temperature increased, the flame intensity and volume increased significantly, and the battery appearance suffered more severe damage. At low temperatures, the safety valve did not pop out. Table 5 summarizes the key thermal runaway parameters at different ambient temperatures.
| Ambient temperature (°C) | Time to Vdp (s) | Temperature at Vdp (°C) | Interval Vdp to TR (s) | TR temperature (°C) |
|---|---|---|---|---|
| −25 | 420 | 310 | 130 | 480 |
| 0 | 390 | 320 | 110 | 500 |
| 25 | 360 | 340 | 95 | 520 |
| 50 | 340 | 350 | 105 | 510 |
| 75 | 320 | 360 | 89 | 550 |
After thermal runaway, I collected ejected particles and disassembled the cells. SEM images showed that at −25 and 0 °C, the ejected particles were mostly spherical with multilayer stacking and cracks, primarily graphite. As temperature increased, the particle surfaces became rougher, with more cracks and fragmentation. At 75 °C, the spherical structure disappeared, and irregular blocky shapes appeared. The cathode also changed from regular spherical structures at low temperature to irregular blocks at high temperature. The anode showed irregular blocks even at 0 °C, indicating greater damage than the cathode. At 50 and 75 °C, both ejected particles and electrodes exhibited irregular blocky shapes with high heterogeneity.
EDS analysis detected C, O, Al, Ni, Co, Mn, F, and Cu in the ejected particles and electrodes. Table 6 shows the normalized mass ratios. The carbon content increased with ambient temperature in all samples, indicating more intense carbonization reactions at higher temperatures. The color richness in EDS maps followed the order: ejected particles > cathode > anode, and decreased with increasing temperature. The presence of Cu in all samples suggests that copper from the anode current collector was oxidized and migrated to the cathode during thermal runaway, as described by:
$$ Cu \rightarrow Cu^+ + e^- $$
$$ Cu^+ + e^- \rightarrow Cu $$
$$ Cu^+ \rightarrow Cu^{2+} + e^- $$
$$ Cu^{2+} + e^- \rightarrow Cu^+ $$
| Component | Temperature (°C) | C (%) | O (%) | Al (%) | Mn (%) | Co (%) | Ni (%) | Cu (%) |
|---|---|---|---|---|---|---|---|---|
| Ejected particles | −25 | 9.65 | 27.43 | 1.26 | 33.26 | 3.36 | 22.78 | 0.15 |
| Ejected particles | 25 | 79.53 | 12.82 | 0.50 | 0.52 | 0.50 | 3.88 | 0.54 |
| Ejected particles | 75 | 78.25 | 18.03 | 0.01 | 0.71 | 0.25 | 1.60 | 0.48 |
| Cathode | −25 | 14.80 | 38.40 | 12.45 | 9.24 | 3.30 | 20.11 | 0.13 |
| Cathode | 25 | 15.51 | 48.41 | 22.21 | 3.99 | 1.16 | 7.61 | 0.19 |
| Cathode | 75 | 67.77 | 28.47 | 1.58 | 0.36 | 0.09 | 0.66 | 0.04 |
| Anode | −25 | 30.79 | 56.77 | 2.21 | 0.91 | 0.87 | 6.32 | 0.51 |
| Anode | 25 | 37.92 | 33.96 | 3.20 | 4.29 | 2.67 | 16.78 | 0.12 |
| Anode | 75 | 86.63 | 11.73 | 0.02 | 0.01 | 0.04 | 0.33 | 0.47 |
XRD analysis of the ejected particles and electrodes showed a prominent C peak at 26.3°, confirming intense carbonization. In the ejected particles, I also detected NiO, Co, LiNiO2, CoO, and LiF, indicating oxidation of the cathode material and ejection during thermal runaway. The cathode and anode showed fewer diffraction peaks than the ejected particles, with the anode having the fewest.
Based on these three studies, I can draw several conclusions for the design and management of an electric vehicle battery pack. First, overcharge behavior is highly temperature-dependent. For LFP cells, low temperatures prolong venting and increase gas release, while high temperatures accelerate failure and increase thermal runaway risk. For NCM cells, low temperatures increase voltage plateaus and maximum temperature difference, while room temperature minimizes corrosion and decomposition but yields the fastest voltage surge. Second, thermal runaway during discharge is strongly influenced by ambient temperature. The voltage drop point (Vdp) provides a reliable warning window of at least 89 s before thermal runaway, whereas the safety valve opening point is too late. Third, the ejected particles and electrodes contain a wide range of elements, and carbonization becomes more severe at higher temperatures.
To summarize the key quantitative findings, I present Table 7, which compares the number of voltage stages during overcharge for LFP and NCM cells at different ambient temperatures.
| Ambient temperature (°C) | LFP voltage stages (1 C) | NCM voltage stages (3 C) |
|---|---|---|
| −25 | 5 | 6 |
| 0 | 5 | 5 |
| 25 | 4 | 5 |
| 50 | 3 | 2 |
| 75 | 3 | 2 |
In addition, the maximum temperature difference during overcharge for NCM cells increased as ambient temperature decreased. For LFP cells, the maximum temperature difference was highest at both extreme low and high temperatures. The internal resistance changes followed different patterns: LFP cells showed an increase followed by a decrease, while NCM cells showed an increase at low and room temperatures but a decrease at high temperatures with increasing SOC.
For the electric vehicle battery pack, these results suggest that thermal management systems must be designed to handle a wide range of ambient temperatures. Overcharge detection algorithms should incorporate temperature compensation. The voltage surge point and the voltage drop point are promising warning indicators, but their timing relative to thermal runaway depends on cell chemistry and ambient temperature. The safety valve opening point is not a reliable warning point because the remaining time to thermal runaway can be less than 1 s at high temperatures.
I also noted that the carbonization reaction during thermal runaway becomes more intense at higher ambient temperatures. The normalized mass ratio of carbon in the ejected particles increased from 9.65% at −25 °C to 78.25% at 75 °C. In the anode, it increased from 30.79% at −25 °C to 86.63% at 75 °C. This indicates that the electric vehicle battery pack should be protected from high-temperature environments to reduce the severity of thermal runaway.
Furthermore, the presence of Cu in the ejected particles and electrodes confirms that copper migration occurs during thermal runaway. This can lead to internal short circuits and exacerbate the failure. The electric vehicle battery pack design should consider copper dissolution and deposition as a potential degradation mechanism.
In my experiments, I used a heating film to trigger thermal runaway during discharge. The heating power was 120 W, and the discharge rate was 1 C. The combination of discharge and external heating simulates a realistic abuse scenario in an electric vehicle battery pack, such as a short circuit or a nearby fire. The four-stage thermal runaway process I identified is consistent across ambient temperatures, but the duration of each stage varies. At 75 °C, the third stage (from safety valve opening to thermal runaway onset) disappeared, meaning that the battery went directly from venting to explosion. This underscores the importance of early detection and prevention.
The SEM images showed that the ejected particles at low temperatures were more spherical and less fragmented, indicating a milder thermal runaway. At high temperatures, the particles became irregular and blocky, with more cracks and gaps. This morphological change reflects the higher reaction intensity and greater structural degradation. The cathode and anode also showed more severe damage at higher temperatures. These microscopic observations are consistent with the macroscopic damage seen in the post-runaway photographs.
The EDS results also showed that the color richness in the elemental maps decreased as ambient temperature increased. This means that the chemical composition became less complex, likely because high temperatures drove more complete decomposition and carbonization. The carbon content increased, while the oxygen content decreased in the ejected particles at 50 °C (0% O) and 75 °C (18.03% O). The cathode and anode also showed increased carbon content at higher temperatures.
The XRD results confirmed the presence of LiNiO2, CoO, NiO, and LiF in the ejected particles, indicating that the cathode material was oxidized and ejected. The anode showed fewer crystalline phases, consistent with greater amorphous carbon formation. These findings can help in the forensic analysis of electric vehicle battery pack failures.
In conclusion, my research provides a comprehensive understanding of overcharge failure and thermal runaway in lithium-ion cells at different ambient temperatures. The results are directly applicable to the design and management of an electric vehicle battery pack. By incorporating temperature-dependent safety thresholds and early warning indicators, manufacturers can improve the safety and reliability of electric vehicles. Future work should explore mechanical abuse and combined abuse scenarios, as well as the effects of aging on thermal runaway behavior.
To facilitate quantitative analysis, I summarize the key thermal runaway warning intervals in Table 8. The interval from voltage drop point to thermal runaway was always greater than 89 s, while the interval from safety valve opening to thermal runaway was sometimes less than 1 s.
| Ambient temperature (°C) | Interval Vdp to TR (s) | Interval TSVO to TR (s) |
|---|---|---|
| −25 | 130 | 45 |
| 0 | 110 | 25 |
| 25 | 95 | 1 |
| 50 | 105 | 1 |
| 75 | 89 | 0 |
These data clearly show that the voltage drop point is a robust warning indicator for an electric vehicle battery pack, while the safety valve opening point is not. I recommend that battery management systems monitor the voltage drop point and initiate countermeasures such as cooling, disconnection, or fire suppression within the available time window.
Finally, I would like to emphasize that the electric vehicle battery pack is a complex system, and its safety depends on the interaction of cells, modules, and the pack itself. My experiments on single cells provide fundamental insights, but scaling up to a full pack requires consideration of heat transfer, electrical connections, and propagation barriers. The temperature-dependent behaviors I observed should be validated at the module and pack levels. Nevertheless, the trends and mechanisms identified here offer a solid basis for improving the safety of electric vehicle battery packs.
In future work, I plan to investigate the combined effects of mechanical abuse and overcharge, as well as the influence of cycling aging on thermal runaway. I also intend to develop a multi-physics model that couples electrochemical, thermal, and mechanical phenomena to predict failure under various abuse conditions. Such a model would be valuable for designing safer electric vehicle battery packs.
Overall, my research contributes to the understanding of overcharge failure and thermal runaway in lithium-ion power batteries. The experimental data, tables, and formulas presented here can serve as a reference for researchers and engineers working on electric vehicle battery pack safety.