Stepwise Fast Charging Strategy and SOH Estimation for Traction Batteries

In the context of accelerating industrialization, the transformation of the automotive sector is reshaping the way people live, while global ecosystems are under ever-increasing stress. The twin challenges of fossil fuel depletion and environmental pollution have pushed the new-energy vehicle (NEV) industry into a period of rapid growth. The continuing decline in the market share of conventional fuel vehicles is driven by the wide adoption of NEVs. At present, pure electric vehicles have become the major consumer segment in the NEV market, and the traction battery is the core energy-storage component and the power source of such vehicles. Among various battery technologies, the ternary lithium-ion battery has attracted enormous attention in the automotive sector due to its high specific energy, outstanding charge/discharge capability and low self-discharge rate. Meanwhile, the sodium-ion battery is emerging as a lower-cost, safer and more cold-tolerant backup or alternative chemistry for automotive traction batteries because it relies on abundant raw materials. In recent years, however, “slow charging” and “inconvenient charging” have become particularly severe, as the construction speed of charging piles has lagged far behind the fleet expansion of electric vehicles. Charging a traction battery quickly and safely has thus become a hot and difficult topic in the charging field. Improving and optimizing the charging protocol can not only relieve charging anxiety, but also support the energy transition and the goal of green, low-carbon, sustainable development.

My research focuses on a stepwise fast-charging strategy for traction batteries and the estimation of their state of health (SOH) under this new charging mode. The central objective is to propose a voltage-cutoff stepwise charging strategy guided by Mas’s laws, differential voltage analysis (DVA) peak changes, and the direct-current internal resistance (DCR) variation during charging. Both cylindrical sodium-ion cells and ternary lithium-ion cells were investigated, and extensive aging-cycle experiments were carried out to evaluate the proposed method against conventional constant-current constant-voltage (CCCV) charging and several capacity-cutoff stepwise charging policies. Finally, the SOH estimation task was addressed by extracting charging-step-sensitive features and using hybrid neural-network architectures.

1. Battery Test Platforms and Experimental Design

The experimental platforms for testing traction batteries were assembled with commercial cyclers, environmental chambers, cell holders, and auxiliary instruments. For the sodium-ion cells, a Newell CT-4008 five-volt/one-hundred-ampere battery tester was used. It records voltage, current, capacity, time and direct-current resistance with an accuracy of ±0.05% of full scale. The temperature chamber was a DGBEL BT-150C with a working range from -40 °C to 150 °C and a control accuracy of ±0.5 °C. For lithium-ion cells, an Arbin BT2000 multichannel battery tester was employed. Each channel has a maximum current of ±10 A, and additional temperature modules were available so that cell-surface temperatures could be logged every two seconds. The lithium tests were performed inside a DGBEL BTT-1000C thermostat, also kept at 25 °C.

The first cell type used in my work was a commercial 18650 sodium-ion cell whose positive electrode was nickel-iron-manganese layered oxide, the negative electrode was hard carbon, and the electrolyte was based on NaPF₆. The second cell type was a commercial 18650 ternary lithium-ion battery with a graphite negative electrode and a LiNiCoMnO₂ positive electrode. Key parameters of the two cells are listed in the table below.

Parameter 18650 sodium-ion cell 18650 lithium-ion cell
Nominal capacity 1400 mAh 1500 mAh
Nominal voltage 3.10 V 3.60 V
Upper/lower voltage 4.00 V / 1.50 V 4.20 V / 2.50 V
AC internal resistance ≤ 18 mΩ ≤ 13 mΩ
Mass 38 g 46 g
Positive material Na-Ni-Fe-Mn layered oxide LiNiMnCoO₂
Negative material Hard carbon Graphite

Before formal cycling, all cells were subjected to a strict screening procedure. The cells were first stored in the environmental chamber for 24 h to equilibrate. I then measured the AC internal resistance with a handheld 1 kHz instrument. Each cell was characterized by a 0.5 C charge-CCCV charge until the upper voltage, followed by a 0.5 C constant-current discharge to the lower voltage. I repeated this sequence three times and selected cells with capacity variation below 0.5% and AC resistance within the ranges given in the next table.

Screening criterion Sodium-ion cell Lithium-ion cell
Discharge capacity 1370–1375 mAh 1505–1510 mAh
AC internal resistance 18.2–18.4 mΩ 12.2–12.4 mΩ

1.1 Rate-capability tests

To understand the capability of the cells at different charging currents, I performed rate-capability charging tests. The sodium cells were charged with a CCCV profile at 0.5 A, 1.0 A, 1.2 A, 1.4 A, 1.6 A and 1.8 A, then discharged at 1 C to 1.5 V. The efficiencies deduced from those tests are summarized below.

Charge current (A) Charge time Charge capacity (mAh) Efficiency (%)
0.5 1:59:14 1372.9 99.59
1.0 1:02:59 1359.6 99.32
1.2 1:11:22 1373.2 99.16
1.4 1:03:11 1404.6 96.99
1.6 0:56:33 1427.1 95.48
1.8 0:51:13 1442.7 94.45

The data show that as the charge current exceeded 1.4 A, the coulombic efficiency dropped below 97% and the apparent charge capacity became larger than the nominal value because of the growing polarization and secondary reactions. Therefore, in the later aging cycling for sodium cells I used 1.0 A (about 0.7 C) for the CCCV control group.

For the lithium-ion cells, I employed two matched cells to avoid high-rate damage during this screening test. One cell was charged at 0.5 A, 1.5 A, 2.5 A, 3.5 A, 4.5 A, 5.5 A and 6.5 A; the other at 1.0 A, 2.0 A, 3.0 A, 4.0 A, 5.0 A and 6.0 A. The discharge current was 1 C (1.5 A) and the cutoff voltage was 2.5 V. Representative results are listed below.

Charge current (A) Charge time Charge capacity (mAh) Efficiency (%) CC phase ratio (%)
1.5 1:09:12 1510.2 99.96 92.16
2.5 0:47:28 1511.0 99.95 86.99
3.5 0:38:07 1511.2 99.94 82.93
4.5 0:32:52 1511.3 99.95 79.56
5.5 0:29:29 1511.8 99.93 76.60
6.5 0:27:09 1514.8 99.97 73.35

The lithium cells showed excellent charge-rate capability with coulombic efficiencies near 100% in all cases. Nevertheless, the constant-current phase ratio decreased significantly as the CC current increased. Above 3 C the CC phase ratio was below 80%, indicating serious polarization at high charging currents.

1.2 HPPC and internal-resistance characterization

In order to guide the stepwise charging design, I performed hybrid pulse power characteristic (HPPC) measurements. Two types of internal resistance were measured: the DC resistance from HPPC pulses and the AC resistance at 1 kHz. For the HPPC test, the cell was charged or discharged for 10 s with a specified current, and the instantaneous voltage changes were recorded. The ohmic resistance and polarization resistance are calculated as

$$R_{0}=\frac{V_{2}-V_{1}}{I_{1}}$$

$$R_{p}=\frac{V_{3}-V_{2}}{I_{1}}$$

where \(V_1\) is the voltage before the pulse, \(V_2\) is the voltage immediately after the pulse is applied, \(V_3\) is the voltage at the end of a 10 s pulse, and \(I_1\) is the pulse current.

For the sodium cells, I performed charge-HPPC tests every 10% SOC over the whole range and then more finely every 2% SOC in the low-SOC region. A pulse current of 1.5 C (2.1 A) was used. The DCR versus SOC curves indicated that the DC internal resistance was highest at very low SOC; below 10% SOC, the internal resistance was about 1.5 times its value at 50% SOC. This observation strongly suggests that charging at low SOC should begin with a reduced current to avoid excessive polarization heating and degradation. No significant increase in DCR was seen at high SOC.

For the lithium cells, I performed charging-HPPC from 0% to 80% SOC every 2% SOC using a 2 C current, and then measured the discharge HPPC resistance from 80% to 0% SOC with the same current. The DCR versus SOC relation was characterized by a U-shaped curve: the DCR was noticeably higher below 10% SOC and again above 90% SOC, while in the middle range it stayed relatively low. Consequently, both low-SOC and high-SOC intervals should be charged with reduced currents.

1.3 Low-rate charging, IC and DV curves

For incremental capacity analysis (ICA) and differential voltage analysis (DVA), the fully discharged cell was placed in a 25 °C chamber for 3 h and then charged at 0.1 C until the upper voltage (4.0 V for sodium, 4.2 V for lithium). The voltage and current were sampled every 10 s. The incremental capacity is defined as

$$\frac{dQ}{dV}=f^{-1}(V)=\frac{I}{dV/dt}$$

and the differential voltage as

$$DV=\frac{dV}{dQ}.$$

The IC curves of both cells exhibit characteristic peaks that correspond to phase transformations in the active materials. The DV curves show valleys and peaks that indicate the voltage intervals where the cell can accept a higher charging current. For the sodium cell, the DV curve is relatively flat between 3.2 V and 3.5 V, and a notable peak appears near 3.5 V. For the lithium cell, the prominent “central graphite peak” appears near 3.9 V. I used these features together with the DCR-SOC characteristics to define the voltage-cutoff stepwise charging procedures.

1.4 Capacity calibration and post-mortem characterization

During the aging tests, capacity calibrations were performed periodically using the full charge/discharge method at 25 °C. The sodium cells were calibrated every 50 cycles, and the lithium cells every 100 cycles. The procedure comprised a 0.5 C constant-current charge to the upper voltage, then a constant-voltage phase until the current dropped to 0.1 C, a 2 h rest, and finally a 0.5 C constant-current discharge to the lower voltage. The second measured discharge capacity was taken as the reference capacity for that cycle.

For the lithium-ion cells, after the 800-cycle aging test I disassembled selected cells inside an argon-filled glove box and analyzed the separator and negative-electrode samples with a field-emission scanning electron microscope (SEM). This post-mortem analysis was used to observe the extent of lithium plating, separator clogging, and electrode structural integrity after the different charging protocols.

2. Development of Stepwise Fast Charging Strategies

2.1 Mas’s laws and the stepwise charging concept

Mas’s three laws describe the acceptable charging current of a battery as a function of its discharge history. The first law can be expressed as

$$a=\frac{K_{1}}{\sqrt{C}},\qquad I=a C=K_{1}$$

where \(K_{1}\) is a current constant, \(C\) is the discharged capacity, and \(a\) is the charge acceptance ratio. The second law and the third law further show that a larger discharge current or a superposition of several discharge processes can increase the acceptable charge current. The ideal “Mas curve” indicates that a fresh battery can accept a relatively high current at low SOC, but the acceptable current gradually decreases as SOC rises. In practice, the theoretical Mas curve can be approximated by a multi-stage constant-current staircase, as depicted in many charging studies.

2.2 Unified charging constraints

I first defined a common set of constraints for all charging strategies so that comparisons would be meaningful. The table below summarizes these constraints.

Constraint Sodium-ion cell Lithium-ion cell
10%–80% SOC charging time < 45 min < 25 min
Maximum temperature rise < 5 °C < 8 °C
Charge efficiency reference > 99% vs 1 C CCCV > 99% vs 2 C CCCV

2.3 Capacity-cutoff stepwise charging strategies

For the sodium-ion cells, I divided the state of charge into 3, 5 and 10 intervals to create three capacity-cutoff stepwise protocols denoted 3SOC-MSCC, 5SOC-MSCC and 10SOC-MSCC. The applied current at each SOC stage and the cutoff condition of each stage are given in the following tables.

3SOC-MSCC sodium cell 0–33% 33–66% 66–100%
Current (A) 1.8 1.4 1.0
5SOC-MSCC sodium cell 0–20% 20–40% 40–60% 60–80% 80–100%
Current (A) 1.0 (until SOC 10%, then 1.8) 1.6 1.4 1.2 1.0

The simpler version is presented for clarity. For the 5-step sodium protocol, from SOC 0–10% the current is 1.0 A; from 10–20% it is 1.8 A; from 20–40% it is 1.6 A; from 40–60% it is 1.4 A; from 60–80% it is 1.2 A; and from 80–100% it is 1.0 A.

10SOC-MSCC sodium cell 0–10% 10–20% 20–30% 30–40% 40–50% 50–60% 60–70% 70–80% 80–90% 90–100%
Current (A) 1.0 1.7 1.6 1.5 1.4 1.3 1.2 1.1 1.0 0.9

All sodium capacity-cutoff protocols switch to constant-voltage charging at 4.0 V when the current was still above zero.

For the lithium-ion cells, I used either three, five, or ten SOC intervals. Some protocols are labelled with suffixes to investigate the influence of different currents under the same cutoff SOC. The following tables summarize the most important capacity-cutoff lithium protocols.

3SOC-MSCC-1 lithium 0–33% 33–66% 66–100%
Current (A) 5.0 3.0 1.5
3SOC-MSCC-2 lithium 0–33% 33–66% 66–100%
Current (A) 4.0 3.0 2.0
5SOC-MSCC-1 lithium 0–20% 20–40% 40–60% 60–80% 80–100%
Current (A) 5.0 4.0 3.0 2.0 1.0
5SOC-MSCC-2 lithium 0–20% 20–40% 40–60% 60–80% 80–100%
Current (A) 4.0 3.5 3.0 2.5 2.0
5SOC-MSCC-3 lithium 0–10% 10–20% 20–40% 40–60% 60–80% 80–100%
Current (A) 2.0 4.0 3.5 3.0 2.5 2.0
10SOC-MSCC lithium 0–10% 10–20% 20–30% 30–40% 40–50% 50–60% 60–70% 70–80% 80–90% 90–100%
Current (A) 2.0 3.6 3.4 3.2 3.0 2.8 2.6 2.4 2.2 2.0

Additionally, a boost-charging profile (BC-CCCV) was defined as 4.0 A constant-current charging from 0% SOC to 3.9 V, then 2.5 A constant-current charging to 4.2 V, and finally a 4.2 V constant-voltage phase until the current fell to 0.1 C.

2.4 Voltage-cutoff stepwise charging strategies

The central idea of the voltage-cutoff method is to use the DV curve and the DCR curve as direct indicators of the battery’s instantaneous ability to accept charge. In the low-DV regions where the voltage changes slowly with respect to capacity, a high charging current is allowed; near DV peaks or when the DCR rises abruptly, the charging current must be reduced.

For the sodium cell I defined the nine-stage voltage-cutoff protocol as follows:

Voltage (V) 2.6 2.8 3.2 3.5 3.8 3.85 3.9 3.95 4.0
Current (A) 1.0 1.4 2.0 1.3 1.2 1.1 0.9 0.7 0.5

The sodium voltage-cutoff strategy is named 9V-MSCC. It starts with a relatively low current of 1.0 A because the cell is at very low SOC with high DCR. After 2.6 V, the current is increased to 1.4 A, and from 2.8 V to 3.2 V the maximum current of 2.0 A is used because the DV curve is flat in that interval. At 3.5 V, near the first DV feature peak, the current is reduced to 1.3 A. From 3.8 V upward the current is progressively decreased to 1.2 A, 1.1 A, 0.9 A, 0.7 A and 0.5 A until the upper voltage of 4.0 V is reached.

For the lithium cell, the voltage-cutoff strategy is denoted 10V-MSCC. The voltage-current relation is listed below.

Voltage (V) 3.6 3.8 3.9 4.0 4.1 4.12 4.14 4.16 4.18 4.2
Current (A) 2.0 5.0 3.5 2.5 2.0 1.5 1.25 1.0 0.75 0.5

In the lithium protocol, the current is initially 2.0 A below 3.6 V because of the relatively high DCR at low SOC. From 3.6 V to 3.8 V the cell enters the low-DV region and I apply the highest current of 5.0 A. Near 3.9 V, which corresponds to the central graphite peak of the DV curve, the current is reduced to 3.5 A. After that the current is gradually stepped down to 2.5 A at 4.0 V, 2.0 A at 4.1 V, and further to 0.5 A at 4.2 V.

2.5 Aging cycling plans

I used the CCCV charging protocol as a control. For the sodium cells the CCCV control was 1.4 A constant-current charging to 4.0 V, followed by a constant-voltage hold at 4.0 V until 0.1 C. For the lithium cells the CCCV control was 3.0 A constant-current charging to 4.2 V, followed by a 4.2 V hold until the charging current was below 0.1 C. All charging steps were followed by a 30 min rest for the sodium cells and a 20 min rest for the lithium cells; then the cells were discharged at 1 C to the lower cutoff. The cycling temperature was kept at 25 °C for both cell types. Aging was continued until 150 cycles for the sodium cells and 800 cycles for the lithium cells, with periodic capacity calibrations as already described.

3. Results of Aging Cycling and Post-Mortem Analysis

3.1 Sodium-ion cell results

The charging time from 10% to 80% SOC is one of the most important fast-charging indicators. In the sodium cells, the fastest protocol was 9V-MSCC, taking only 38 min 10 s, while the CCCV control required 45 min 26 s. The relative reductions are summarized below.

Protocol 10–80% SOC time Saved time Relative reduction
CCCV 45 min 26 s — —
3SOC-MSCC 41 min 54 s 3 min 32 s 7.78%
5SOC-MSCC 41 min 11 s 4 min 15 s 9.35%
10SOC-MSCC 43 min 00 s 2 min 26 s 5.36%
9V-MSCC 38 min 10 s 7 min 16 s 16.0%

After 150 cycles, the SOH values measured on the sodium cells under each protocol are presented below.

Protocol SOH after 150 cycles (%)
CCCV 84.9
3SOC-MSCC 85.7
5SOC-MSCC 90.7
10SOC-MSCC 90.9
9V-MSCC 92.3

The 9V-MSCC protocol improved the final SOH by 7.4 percentage points compared with the CCCV control. The 5SOC-MSCC and 10SOC-MSCC results were almost identical, suggesting that increasing the number of capacity-cutoff stages beyond five supplies diminishing benefit. In contrast, the 3SOC-MSCC protocol was not much better than CCCV, since the high current in the first 33% SOC interval was applied while the DCR was still large and the SOC region was not appropriate for high-rate charging.

I also analyzed the incremental capacity curves of aged sodium cells. The IC peak positions and heights are listed in the table below.

Protocol 2nd peak voltage (V) 2nd peak height (mAh/V) 3rd peak voltage (V) 3rd peak height (mAh/V)
CCCV 2.8721 1478.8 2.9251 2309.7
3SOC-MSCC 2.8635 1598.4 2.9235 2327.7
5SOC-MSCC 2.8578 1649.1 2.9194 2446.5
10SOC-MSCC 2.8584 1649.5 2.9197 2460.6
9V-MSCC 2.8580 1704.8 2.9199 2502.1

9V-MSCC clearly produced the least fading of the IC peaks, followed by 5SOC-MSCC and 10SOC-MSCC. The largest fade, especially in the second IC peak, was seen under CCCV and 3SOC-MSCC.

The internal-resistance results after 150 cycles are summarized below.

Protocol DCR at 3.55 V (mΩ) AC internal resistance (mΩ)
CCCV 116.0 27.8
3SOC-MSCC 113.1 27.6
5SOC-MSCC 105.6 25.4
10SOC-MSCC 103.6 25.6
9V-MSCC 98.5 23.5

The 9V-MSCC strategy successfully reduced both DC and AC resistance growth. This confirms the importance of lowering the charging current at high-DCR phases and near the DV peak.

3.2 Lithium-ion cell results

For the lithium-ion cells, the 10%-80% charging times and full charging times for all protocols are listed in the following table.

Protocol 0–100% SOC time 10–80% SOC time
CCCV-3A 41 min 46 s 21 min 03 s
BC-CCCV 41 min 16 s 20 min 16 s
3SOC-MSCC-1 45 min 05 s 22 min 18 s
3SOC-MSCC-2 42 min 31 s 21 min 15 s
5SOC-MSCC-1 47 min 53 s 21 min 30 s
5SOC-MSCC-2 42 min 11 s 20 min 36 s
5SOC-MSCC-3 44 min 31 s 20 min 54 s
10SOC-MSCC 44 min 05 s 21 min 16 s
10V-MSCC 45 min 38 s 21 min 09 s

After 800 cycles, the SOH values under all charging strategies are compared in the table below. 10V-MSCC achieved the highest SOH of 89.5%, whereas the CCCV control had already declined to 64.1%.

Protocol SOH after 800 cycles (%)
CCCV 64.1
BC-CCCV 68.7
3SOC-MSCC-1 60.1
3SOC-MSCC-2 74.9
5SOC-MSCC-1 76.7
5SOC-MSCC-2 78.6
5SOC-MSCC-3 79.5
10SOC-MSCC 79.7
10V-MSCC 89.5

The AC internal resistance of the lithium cells after 800 cycles is presented below. The lowest increase was again obtained with 10V-MSCC.

Protocol AC internal resistance after 800 cycles (mΩ)
CCCV 21.32
BC-CCCV 21.11
3SOC-MSCC-1 21.53
3SOC-MSCC-2 19.76
5SOC-MSCC-1 19.95
5SOC-MSCC-2 19.65
5SOC-MSCC-3 19.17
10SOC-MSCC 19.08
10V-MSCC 18.57

The 3SOC-MSCC-1 protocol caused more damage than the CCCV control because its initial 5 A charging current was excessive in the low-SOC region with high internal resistance. This trend confirms the importance of tailoring the first charging step according to the DCR-SOC behavior.

SEM observations after 800 cycles strongly support the quantitative data. Under CCCV, the separator was severely clogged and the fibrous network collapsed; the graphite negative electrode had numerous lithium dendrites, many with lengths exceeding 3 μm. Under 5SOC-MSCC-2, the separator was partially damaged, and a few short dendrites around 1 μm were present. Under 10V-MSCC, the separator retained a regular fibrous structure and the graphite particles remained crisp and closely packed, with almost no dendrite growth. These microstructural results provide direct evidence that the voltage-cutoff stepwise protocol suppresses the degradation of the traction battery during fast charging.

4. SOH Estimation for Voltage-Cutoff Stepwise Charging

After obtaining the long-term cycling data, I turned to the second important topic of this thesis: state-of-health estimation under the new voltage-cutoff stepwise charging protocol. The study was focused on the 9V-MSCC protocol for sodium cells and the 10V-MSCC protocol for lithium cells.

4.1 Feature extraction

I first plotted the charge capacity versus voltage curves for different cycle numbers during the voltage-cutoff charging process. For both the sodium and the lithium cells, a clear degradation trend appears: the whole capacity-voltage curve shifts to the left as the cell ages. More importantly, the first three charging stages show the largest distinction between consecutive cycle blocks. Because the currents in these first stages are relatively high, any loss of active material or impedance increase directly changes the charge capacity stored in each voltage interval. The later steps have lower currents and therefore produce a smaller signal for SOH estimation.

For the sodium 9V-MSCC protocol, the selected health features are listed below. The first three features are the charging times of the first three stages; the remaining features are the total charging time, the DC charging resistance from a calibration HPPC, and the median charging voltage.

Feature Description
H1 First-stage charging time
H2 Second-stage charging time
H3 Third-stage charging time
H4 Total charge time
H5 DC charging resistance
H6 Median charge voltage

For the lithium 10V-MSCC protocol, I used the charged capacities and endpoint temperatures of the first three voltage stages as the base feature set. This set is called Plan 1. To examine whether selecting only the first three stages is adequate, I also built a second feature set, Plan 2, which includes the same three-stage features plus the charged capacities and endpoint temperatures of stages 4, 5 and 6.

Feature Description
F1 First-stage charged capacity
F2 First-stage end temperature
F3 Second-stage charged capacity
F4 Second-stage end temperature
F5 Third-stage initial voltage slope
F6 Third-stage charged capacity
F7 Third-stage end temperature

4.2 Correlation analysis

For the sodium cells, I quantified the linear correlation between the features and capacity using the Pearson correlation coefficient:

$$\rho_{X,Y}=\frac{\operatorname{cov}(X,Y)}{\sigma_{X}\sigma_{Y}}
=\frac{\sum (x_i-\bar{x})(y_i-\bar{y})}
{\sqrt{\sum (x_i-\bar{x})^2 \sum (y_i-\bar{y})^2}}$$

The absolute values of the Pearson coefficients between H1–H6 and capacity were all higher than 0.9, confirming that the selected features are strongly related to SOH.

For the lithium cells, because the capacity fade was monotonic but not completely linear over 800 cycles, I used the Spearman rank correlation coefficient:

$$\rho_{s}=1-\frac{6\sum d_i^2}{n(n^2-1)}$$

where \(d_i\) is the rank difference between the feature and capacity. The absolute Spearman coefficients for F1–F7 were also found to be greater than 0.9.

4.3 PSO-BP algorithm for sodium-ion cells

For the sodium 9V-MSCC protocol, I developed a hybrid health-estimation model based on a back-propagation neural network whose initial weights and thresholds were optimized by particle swarm optimization. The structure has six input neurons, one hidden layer with a number of neurons determined by the empirical formula

$$m=\sqrt{n+p}+a$$

where \(n\) is the number of input features, \(p\) is the number of output neurons (one SOH value), and \(a\) is an integer between 1 and 10. The position and velocity of every particle are updated with

$$v_{id}^{(t+1)}=\omega v_{id}^{(t)}+c_{1}r_{1}(p_{id}^{(t)}-x_{id}^{(t)})+c_{2}r_{2}(p_{gd}^{(t)}-x_{id}^{(t)})$$

$$x_{id}^{(t+1)}=x_{id}^{(t)}+v_{id}^{(t+1)}$$

The fitness of the particle is the mean square error between the estimated and actual SOH. After PSO searches for the optimal weights and thresholds, the BP network performs fine-tuning with gradient descent. The model was trained separately on 70% and 50% of the available early-cycle samples and evaluated on the remaining samples.

I evaluated the model by mean absolute error and root mean square error:

$$\mathrm{MAE}=\frac{1}{n}\sum_{i=1}^{n}|y_i-\hat{y}_i|$$

$$\mathrm{RMSE}=\sqrt{\frac{1}{n}\sum_{i=1}^{n}(y_i-\hat{y}_i)^2}$$

The estimation results for the sodium 9V-MSCC battery under different training-set ratios are summarized below, along with comparisons against SVM, ELM, CNN, BP and GA-BP.

Method Training set RMSE (%) MAE (%)
PSO-BP 70% 0.610 0.450
50% 0.678 0.583
GA-BP 70% 0.873 0.647
50% 0.910 0.739
BP 70% 1.326 1.113
50% 2.182 2.043
CNN 70% 2.150 2.076
50% 3.217 2.043
ELM 70% 2.571 2.024
50% 4.349 3.722
SVM 70% 1.445 1.220
50% 4.012 3.230

PSO-BP consistently outperformed the other methods. Even when the training set was reduced to 50% of the early data, the RMSE remained below 0.7%. This indicates that the voltage-cutoff stepwise charging features embedded in the first three charging stages are robust health indicators for sodium traction batteries.

4.4 CNN-LSTM algorithm for lithium-ion cells

For the lithium 10V-MSCC protocol, I used a hybrid convolutional neural network combined with long short-term memory layers. The CNN layers are responsible for extracting local patterns in the multi-feature input, while the LSTM layers model the temporal dependencies through their forget gate, input gate, and output gate. The LSTM updating procedure is described by

$$f_{t}=\sigma(W_{f}[h_{t-1},x_{t}]+b_{f})$$

$$i_{t}=\sigma(W_{i}[h_{t-1},x_{t}]+b_{i})$$

$$\tilde{C}_{t}=\tanh(W_{C}[h_{t-1},x_{t}]+b_{C})$$

$$C_{t}=f_{t}\odot C_{t-1}+i_{t}\odot \tilde{C}_{t}$$

$$o_{t}=\sigma(W_{o}[h_{t-1},x_{t}]+b_{o})$$

$$h_{t}=o_{t}\odot \tanh(C_{t})$$

The CNN-LSTM model was compared to standalone LSTM and PSO-BP for both Plan 1 and Plan 2 feature sets. The resulting errors are given in the following table.

Model Feature plan RMSE (%) MAE (%)
CNN-LSTM Plan 2 0.856 0.681
Plan 1 0.929 0.829
PSO-BP Plan 2 0.848 0.571
Plan 1 1.304 0.988
LSTM Plan 2 1.975 1.529
Plan 1 2.360 1.946

With the complete Plan 2 features, CNN-LSTM and PSO-BP achieved similar accuracy. But when only the first three charging stages were used, CNN-LSTM remained very accurate and clearly outperformed PSO-BP and LSTM. This result has an important practical meaning: it is possible to estimate the SOH of a traction battery under 10V-MSCC charging as early as the end of the third charging stage, which occurs approximately 13 minutes after the beginning of charging. Earlier SOH information enables the battery management system to adapt the remaining charging steps or to report a reliable health estimate before the fast-charging event is completed.

5. Conclusion and Outlook

In my thesis I carried out a comprehensive study on stepwise fast-charging strategies for two representative power-cell chemistries used in traction batteries: sodium-ion cells and ternary lithium-ion cells. By combining Mas’s law, differential voltage analysis, and the measured charging DC resistance, I designed a voltage-cutoff stepwise protocol that avoids the high-DCR low-SOC region and the sensitive DV peaks during high-rate charging.

The major conclusions can be summarized as follows:

  1. The voltage-cutoff stepwise protocols, 9V-MSCC for sodium cells and 10V-MSCC for lithium cells, provided the shortest charging time in the sodium case and the best capacity retention in both chemistries.
  2. After 150 cycles, the sodium-ion cells charged with 9V-MSCC had a SOH of 92.3%, which was 7.4 percentage points higher than that of the CCCV control. After 800 cycles, the lithium-ion cells charged with 10V-MSCC had a SOH of 89.5%, 25.4 percentage points above the 2C-CV benchmark.
  3. The DC and AC internal-resistance growth were minimized under the voltage-cutoff strategy. SEM analysis confirmed that 10V-MSCC preserved a clean separator and a dendrite-free graphite negative electrode, while CCCV charging produced severe separator clogging and lithium dendrites.
  4. For the new charging modes, the history of the first three voltage stages carries strong health-related information. Pearson and Spearman analyses proved that these features are highly correlated with capacity.
  5. The PSO-BP model estimated the SOH of sodium 9V-MSCC cells with RMSE less than 0.68% even with only 50% training data. The CNN-LSTM model estimated the SOH of lithium 10V-MSCC cells with RMSE less than 0.93% using only the first three charging stages, allowing an early and precise SOH estimate.

There are several directions that deserve future work. The voltage thresholds of the proposed voltage-cutoff protocol may need to be adapted as the cell ages, because the DV curve itself changes with degradation. My sodium-cell tests were limited to 150 cycles because the 4.0 V cutoff was relatively high for the tested sodium chemistry, and no temperature or post-mortem analysis was available for those cells. Future experiments should include thermal monitoring and post-mortem imaging for sodium cells. Furthermore, SOH estimation models should be extended to the other capacity-cutoff protocols and to more realistic fast-charging profiles that include varying ambient temperatures and dynamic current patterns. In conclusion, the voltage-cutoff stepwise strategy is a promising route for safe, low-degradation fast charging of future traction batteries, and the hybrid-data-driven SOH estimators developed in this work can support real-time onboard battery management.

Scroll to Top